GENERAL PROPERTIES
| |
| PHYSICAL |
|
SIZIN
1 |
SIZIN
2 |
SIZIN
S |
| |
| Density |
Kg/dm3 |
6,7 |
6,6 |
6,6 |
| Melting range |
°C |
380÷390 |
353÷358 |
360÷365 |
| Specific heat capacity |
J/Kg°K |
418,6 |
418,6 |
418,6 |
| Thermal conductivity at 20°C |
W/m°K |
104 |
104 |
104 |
| Optimum casting range |
°C |
420÷430 |
390÷400 |
380÷420 |
| Thermal linear expansion |
cm/cmx10-6/°C |
27,7 |
28,0 |
- |
| Linear shrinkage |
% |
1,085 |
1,085 |
1,080 |
| Maximum casting temperature |
°C |
450 |
425 |
450 |
| |
| |
| CHEMICAL (test%) |
|
SIZIN
1 |
SIZIN
2 |
SIZIN
S |
| |
| Aluminium |
|
3,9÷4,3 |
3,9÷4,3 |
4,0÷4,6 |
| Copper |
|
2,7÷3,5 |
2,7÷3,5 |
2,8÷3,1 |
| Magnesium |
|
0,09÷0,14 |
1,80÷2,20 |
0,50÷0,70 |
|
|
|
|
|
| Impurities: |
Lead |
max 0,003 |
max 0,003 |
max 0,003 |
|
Cadmium |
max
0,003 |
max
0,003 |
max
0,003 |
|
Tin |
max 0,001 |
max 0,001 |
max 0,001 |
|
Iron |
max 0,030 |
max 0,030 |
max 0,030 |
|
Zinc |
remainder |
remainder |
remainder |
| |
| |
MECHANICAL
(the values refer to the cast item) |
SIZIN
1 |
SIZIN
2 |
SIZIN
S |
| |
|
|
Sand
casting
|
| Tensile strength |
MPa |
200-220 |
160-180 |
200-250 |
| Linear elongation |
% |
1,0-1,5 |
molto
basso |
- |
| Brinell hardness (500 kg) |
HB |
105-110 |
145-150 |
145-150 |
| Tensile strength at
compression (0,1%) |
MPa |
800-850 |
680 |
700 |
| |
|
|